Stabilor® NF IV 

Technical data

Type: extra hard, Type 4 acording to ISO 1562
Colour: bright-yellow

Compositions in

weight-%

Gold/Platin metals

65,0

Gold (Au)

55,0 

Palladium (Pd) 9,9

Silver (Ag)

29,0

Zinc (Zn)

1,0

Tin (Sn) 

1,0

Indium (In)

4,0 

Iridium (Ir)

0,1

 

    europaflagge

Information presented on  this webpage only refers  to European Markets.

Melting range  (°C)   940 - 1065 
Vickers hardness  (HV 5)   w 150   a 220   g 205
0,2 %-yield strength** (N/mm2)   a 555   g 440
Tensile strength** (N/mm2)   a 640   g 570
Elongation**  (%)   a 3   g 3

Density (g/cm3)   13,8

** measurements with samples according to ISO 1562, 9693, 8891
w = soft
a = hardened
b= attainable hardness due slow cooling in the mould

 
 
 